Rated on 5 criteria: print temperature, warping, strength, creep resistance, and heat resistance (★1-5).
Nozzle: 220-250°C
Bed: 70-80°C
Moderate warping
Bending Strength: 76.69 MPa
Rated
Heat Resistance Temp: 75°C
| Item | Recommended Value | Notes |
|---|---|---|
| Nozzle Temperature | 220-250°C | Lower temp for transparency |
| Bed Temperature | 70-80°C | For better adhesion |
| Fan Setting | 30-50% | Too strong causes poor layer adhesion |
| Print Speed | 30-50mm/s | Slow speed prevents stringing |
| Nozzle Diameter | 0.4-0.6mm | 0.6mm reduces stringing |
| Caution | Prone to stringing, retraction adjustment required | |
| Item | Measured Value |
|---|---|
| Default (Flat Layout) | |
| Bending Strength | 76.69 MPa |
| Flexural Modulus | 2033 MPa |
| Z-Axis Strength (Vertical Layout) | |
| Bending Strength | 26.59 MPa |
| Flexural Modulus | 1703 MPa |
| Test Method | 3-Point Bending Test(Details) |
Bending test data for this filament has not been registered yet.
The graph will be displayed once data is added.
Various derivative filaments with enhanced properties have been developed based on PETG. Choose the optimal one according to your application.
• Prone to stringing, optimizing retraction settings is important.
• Bed adhesion may be too strong, be careful when removing prints.
• High-temperature printing requires adequate ventilation.
• For transparency, set printing temperature lower.